Along with hardware characterized by top performance shipbuilding steel, POSCO offers software represented by steel use skills consisting of welding and performance evaluation
Application Technology generally adapted for parts is described below. Please contact us through ¡®Contact Us > Q&A' for more details.
Brittle Crack Arrest Method for Ultra Large Containership
Brittle Crack Arrest(BCA) Steels (EH40/47BCA, EH40/47BCACOD)
Prevent the unstable brittle fracture in weld joint of upper deck and Hatch-side coaming
Using the brittle crack arrest toughness excellent steel
Applicaiotn of brittle crack arrest design
Prevention of unstable fracture by applying a brittle crack arrest steels and design
Strucural steels for shipbuilding : EH/DH32-TMU, EH36-TMU, EH40-TMU
Development of high heat input welding technology for 1 pass welding of thick plates (max.85mm)
Improvement of welding productivity for ultra large container with very thick plates
E500(EH51)-TM
High adaptability for Arctic region by using high performance steel for low temperature service
Suggestion of welding consumables and welding conditions by evaluation of cold crack
susceptibility of welded joint with heat input range 1.0~5.0kJ/mm
TS (MPa) | Preheating temp. (¨¬C) | ||
---|---|---|---|
0 | RT | ||
1.0kJ/mm | Wire 1 | No-Crack | No-Crack |
Wire 2 | No-Crack | No-Crack | |
1.7kJ/mm | Wire 2 | No-Crack | No-Crack |
Wire 1 | No-Crack | No-Crack |
Grade | Location | YP (MPa) | TS (MPa) | EL (%) | CVN@-40¨¬C[J] | CTOD@-20¨¬C [mm] |
---|---|---|---|---|---|---|
E500 (50t) | Head | 552 | 658 | 21.3 | 300~450 | 2.23/3.13 /3.19 |
Tail | 557 | 663 | 22.5 | |||
Requirement | ¡Ã 500 | ¡Ã 0.25 |
Application on ship design for low temperature service
Weight reduction by using high strength steel